Synthesis and Characterization of PSS Doped Tetraaniline Nanorods via Soft-Template Assisted Method
K. Basavaiah*, and A.V. Prasada Rao
Department of Inorganic and Analytical Chemistry, Andhra University, Visakhapatnam -530003, India.
*Corresponding Author E-mail: klbasu@gmail.com
ABSTRACT:
Tetraaniline nanorods have been synthesized by emulsion polymerization method using long alkyl chain organic acid, poly (styrenesulfonic acid), PSS as dopant as well as soft-template. The resulting tetraaniline nanorods were characterized by UV-visible spectroscopy, Fourier transform infrared spectroscopy, scanning electron microscopy and thermogravimetric analysis. The results indicated that the successful formation of tetraaniline rods. The morphologies of tetraniline were found to be dependent on molar ratios of N-phenyl-1, 4-phenylenediamine to PSS. Thermogravimetry data revealed that the PSS doping improved the thermal stability of tetraaniline.
KEYWORDS: Conducting polymers, nanotubes, soft-template, tetraaniline, thermal stability.
INTRODUCTION:
In the past decade, conjugated polymer-based electrochromic materials have attracted great attention because of their low cost, ease of processing, and relatively high optical contrast and response speed, which are essential for their applications in electrochromic devices.1-4 Among all conjugated polymers, polyaniline (PANI) has been emerged as a potential candidates for many technological applications due to its good environmental stability, high electrical conductivity, unique redox chemistry, easy synthesis and control of the electronic and optical properties by the degree of oxidation and protonation5 It has been used in applications such as organic lightweight batteries, microelectronics, electrorheological fluids, and chemical sensors.6-10 Moreover, PANI exhibits a large spin density so interesting electrical and magnetic properties arise that are highly dependent on the doping level and the structure of the polymer. However, like many other conducting polymers, PANI is intractable and suffers from poor processability, mainly because of its rigid, highly conjugated backbone. Many methods have been explored to overcome their poor processability of PANI includes, template-synthesis, electron-spinning, interfacial polymerization, electrochemical polymerization and template-free method.11-15 Among these methods, the emulsion polymerization method16 has attracted much attention due to its simplicity. In this technique, long alkyl chain organic acid is used as dopant as well as soft-template for PANI dispersions.
Compared to the parent polymer, oligomers of aniline have received far less attention. Reports on aniline oligomers focus mainly on organic synthetic routes to an oligomeric material possessing a bulk, granular morphology. Furthermore, their properties are generally studied experimentally and theoretically to serve as model compounds for polyaniline. Despite the rapid developments in nanostructured polyaniline, little effort has been invested in investigating oligoaniline nanostructures. Among, PANI oligomers, tetraaniline is most attracted attention because soluble in common solvents, exhibit similar electroactivity as PANI, and have well-defined structure, designed end group, and monodispersed molecular weight.17The most interesting form of PANI is emeraldine, which has ca. 50% amine and ca. 50% imine nitrogen, that is one of 4 rings is quinoid, the remaining three being benzoid. Hence, tetraaniline is perfect model compound for PANI since its chemical structure resemble to the EBPANI.
In this paper, we present the preparation of polystyrene sulfonic acid (PSS) doped tetraaniline nanorods via soft-template method. Here, PSS acts as dopant as well as soft template for tetraaniline nanostructures. The effect of molar ratios of N-phenyl-1, 4-phenylenediamine to PSS was investigated.
MATERIALS AND METHODS:
Preparation of Tetraaniline nanorods:
Polystyrene sulfonic acid (PSS) doped tetraaniline was synthesized via soft-template method, in which PSS and aqueous ammonium persulphate were used as surfactant and oxidant, respectively. In a typical procedure, 0.1839 g N-phenyl-1, 4-phenylenediamine and 1.9105 g of PSS were dissolved in 50 ml of distilled water in round bottom flask with constant stirring for 2h at 0-5 0 C. A pre-cooled, equimolar solution (1mol/L) 1 ml ammonium persulphate was added to the reaction mixture to initiate the polymerization of N-phenyl-1, 4-phenylenediamine with constant stirring at 0-5ºC. After addition of oxidant, reaction mixture was allowed to proceed for another 5 h at 0-5ºC. The colour of the reaction mixture was slowly changes from a colourless, to light blue and then to a dark green, which is indicative of formation of PSS doped tetraaniline. The resulting precipitate was filtered and washed with distilled water and methanol. Finally, the product was dried under vacuum at room temperature for 12 h. The same procedure has been adopted for preparation of all PSS doped tetraaniline while varying the molar ratio of N-phenyl-1, 4-phenylenediamine to PSS from 1:1 to 1:5.
Characterization:
The UV-Visible absorption spectra of the samples were recorded on a Perkin-Elmer double beam LS-50 spectrophotometer. The samples were dissolved in dry dimethylsulphoxide (DMSO) and centrifuged to remove any undissolved polymer. The clear solutions were taken in quartz cuvettes. The infrared spectra were recorded over the range 4000 - 400 cm-1 in a Perkin-Elmer Model SPECTRUM 1000 FTIR spectrometer. The powdered samples were mixed thoroughly with KBr and pressed into thin pellets. Morphology of PSS doped tetraaniline was studied by scanning electron microscopy (SEM).Thermal stability of nanocomposite samples was determined from thermogravimetric analysis (TGA, Cahn TG131) with a heating rate of 20 degree per minute under N2 atmosphere.
RESULTS AND DISCUSSIONS:
Tetraaniline nanorods have been prepared by using APS as an oxidant in presence of PSS via soft template method. The formation mechanism of PSS doped tetraaniline nanorods shown in schematic illustration 1.Here, PSS is expected to play dual role in the formation of composites as a dopant for tetraaniline as well as a surfactant to form micelles during the polymerization due to the presence of hydrophobic and hydrophilic parts (-SO3H groups of PTSA). Here, N-phenyl-1, 4-phenylenediamine is hydrophobic. In an aqueous solution containing mixture of N-phenyl-1, 4-phenylenediamine and PSS, a complex formation is expected due to acid–base type interactions between the –SO3H group in PSS and –NH2 group in. This anilinum –PSS complex acts as site for growth of tetraaniline nanostructures. Further, the N-phenyl-1, 4-phenylenediamine –PSS complex could self assembled into nanorods.
Scheme1. Schematic illustration of formation mechanism of PSS doped tetraaniline nanorods .
Molecular structure of PSS doped tetraaniline was characterized by UV-Visible spectroscopy, Fourier-transform infrared (FTIR) spectroscopy and X-ray diffraction pattern (XRD). Fig. 1. Shows the UV-Visible spectra of PSS doped tetraaniline which is in complete agreement with literature reports.18-19
Figure.1. UV-Visible spectra of PSS doped tetraaniline nanorods prepared at 1: 5 molar ratio of N-phenyl-1, 4-phenylenediamine to PSS.
The UV-Visible absorption spectrum in dimethyl sulfoxide (DMSO) showed three distinct bands at 330 and 685 nm. Absorption bands at 330 and 685 nm have been assigned to π →π * transition of benzenoid rings in the tetraaniline chain and the transition caused by inter chain charge transfer from two adjacent benzenoid ring to the quinoid ring of tetraaniline chain respectively. Both absorbance bands of tetraaniline were blue shifted from those of pure tetraaniline, indicating that the there is some interaction between PSS and tetraaniline backbone.
The FT-IR spectra (Figure.2) of the synthesized tetraaniline samples were in good agreement with the earlier reports on tetraaniline.[20-24] The peaks at 3163, 1589 and 1496 cm-1 attributed to N-H stretching vibration, C=C stretching of quinoid phenyl and benzenoid phenyl rings, respectively. The peak at 1404 is due to stretching frequency of B-N=Q moiety (B refers to benzenoid and Q refers to quinoid ring). The presence of this peak confirms that the formation of phenazine units. These phenazine units acts as initiation sites for the growth of tetraaniline tubes indicating self-assembly of phenazine units as previously reported by Trchova et al. is partially doped with PSS, while completely absent in fully doped tetraaniline.The peak at 1307 cm-1 is assigned to C-N stretching vibrations of the 1, 4- disubstituted benzene ring of tetraaniline. The peaks at 1167 and 1132 cm-1 attributed to N=Q=N modes of tetraaniline and PSS respectively. The peaks at 1035, 617 and 1008 cm-1 are due to symmetric and asymmetrical vibrations of O=S=O, S-O, S-C and C-H of PSS respectively, indicating the presence of the sulfonate group. Sulfonate group of PSS interact with protanated imine nitrogen in neighbouring chain and stabilize tetraaniline in the form of nanotubes by ionic bonding. In addition to the characteristic tetraaniline peaks, FTIR spectra of tetraaniline nanotubes showed additional peak at 831 cm-1, which can be ascribed to C-H out of plane bending of 1,4-disubstituted benzene rings of tetramer
Figure.2. FTIR spectra of PSS doped tetraaniline nanorods prepared at 1: 5 molar ratio of N-phenyl-1, 4-phenylenediamine to PSS.
Figure.3. shows SEM images of the PSS doped tetraaniline prepared at different molar ratios of N-phenyl-1, 4-phenylenediamine to PSS. The morphologies of tetraaniline were critically depended upon molar ratio of N-phenyl-1, 4-phenylenediamine to PSS SEM images revealed that the nanorod morphology for PSS doped tetraaniline prepared at molar ratio 1:5 of N-phenyl-1, 4-phenylenediamine to PSS. The particular morphologies were formed for other molar ratio of N-phenyl-1, 4-phenylenediamine to PSS. It could be believed that the excess of PSS induce the formation of nanorods via self-assembly process.
Figure 4. Shows a TG-DTG curve for PSS doped tetraaniline nanorod prepared at 1:5 molar ratio of N-phenyl-1, 4-phenylenediamine to PSS. TG-DTG is recorded under N2 flow at a heating rate of 20ºC per minute from 50-850 0C.Three main inflection regions can be observed. The first region at lower temperatures (<100ºC) is due to removal water, and other volatiles in tetra aniline nanorod. The unbound PSS loss below 300ºC . The weight loss in temperature range of 300-500ºC can be ascribed to the removal of bound PSS and decomposition of tetraaniline chain. The third weight loss region of 500-840ºC is due to decomposition of tetraaniline chain. Thermal studies indicated that thermal decomposition of tetraniline chain occurs at higher temperature for PSS doped tetraaniline nanorod as compared to undoped tetraaniline.
Figure.3. SEM images of PSS doped tetraaniline nanorods prepared at different molar ratio of N-phenyl-1, 4-phenylenediamine to PSS.
Figure.4. TG-DTG of PSS doped tetraaniline nanorods prepared at 1: 5 molar ratio of N-phenyl-1, 4-phenylenediamine to PSS.
CONCLUSIONS:
In summary, we have demonstrated a simple, reproducible, and facile method of preparation of tetraaniline nanorod via micellar assisted method using PSS as dopant as well as soft template. The morphology of tetraaniline was depended on molar ratio of N-phenyl-1, 4-phenylenediamine to PSS. The PSS- anilium complex act as nucleation site for growth of tetraaniline nanorods. The spectroscopic data established the interaction between PSS and tetraniline. TG data indicated that PSS doping improved the thermal stability of tetraaniline nanorods.
ACKNOWLEDGEMENTS:
This work was supported by University Grants Commission (UGC-India), New Delhi, India under project grant No. MOES/11-MRDF/1/28/P/08).
REFERENCES:
1. Mortimer, R. J.; Dyer, A. L.; Reynolds, J. R. Displays, 27: 2006: 2.\
2. Jagur-Grodzinski, J. Polym. Adv. Technol., 13:2002: 615.
3. Argun, A. A.; Aubert, P. H.; Thompson, B. C.; Schwendeman, I.;Gaupp, C. L.; Hwang, J.; Pinto, N. J.; Tanner, D. B.; MacDiarmid,A. G.; Reynolds, J. R. Chem. Mater. , 16: 2004: 4401.
4. Yildiz, U. H.; Sahin, E.; Akhmedov, I. M.; Tanyeli, C.; Toppare, L. J. Polym. Sci., Part A: Polym. Chem., 44: 2006 : 2215.
5. (a) MacDiarmid, A. G. Synth. Met. , 84: 1997: 27. (b) Chen, W.-C.; Jenekhe, S. A. Macromolecules, 25: 1992: 5919. (c) Chinn, D.; DuBow,J.; Liess, M.; Josowicz, M.; Janata, J. Chem. Mater., 7 :1995 : 1504.
6. Tsutsumi, H.; Yamashita, S.; Oishi, T. J. Appl. Electrochem., 27: 1997: 477.
7. Paul, E. W.; Rico, A. J.; Wrighton, M. S. J. Phys. Chem., 89 : 1985 :1441.
8. Lee, Y. H.; Kim, C. A.; Jang,W.H.; Choi, H. J.; Jhon, M. S. Polymer, 42 :2001 :8277.
9. Sangodkar, H.; Sukeerthi, S.; Srinivasa, R. S.; Lal, R.; Contractor, A. Q. Anal. Chem. , 68 :1996 :779.
10. Bossi, A.; Piletsky, S. A.; Piletska, E. V.; Righetti, P. G.; Turner, A. P. F. Anal. Chem. , 72 : 2000 :4296.
11. Martin C R Chem. Mater. , 8 1 : 1996 :739–1746.
12. Reneker D H and Chun I, Nanotechnology, 7: 1996 : 216–223.
13. Zhang X, Goux W J and Manohar S K , J. Am. Chem. Soc. , 126 : 2004: 4502–4503.
14. He Y, Mater. Sci. Eng. B, 122 : 2005 : 76–79.
15. Liang L, Liu J, Windisch C F Jr, Exarhos G J and Lin Y, Angew. Chem. Int. Edn., 41: 2002: 3665–3668.
16. Wan M and Li J, J. Polym. Sci. A, 37 : 1999: 4605–4609.
17. Wei, Y.;Yu, Y.; Zhang,W.;Wang, C.; Jia, X.; Jansen, S. A, Chin. J.Polym. Sci. , 20 : 2002: 105–118.
18. M. X. Wan, Synth.Met, 31: 1989: 51.
19. G. Venugopal, X.Quan, G.E. Johnson, F.M.Houlihan, E. Chin, O.nalamasu, Ce. Mater, 7 : 1995 : 271.
20. M. Trchova, I. Sedenkova, E.N. Konyushenko, J. Stejskal, P.Holler, G.C.I.Marjanovic, J. Phys. Chem. B., 110: 2006: 9462-9468.
21. S,-A, Chen, H.T. Lee, Macromolecules, 28: 1995: 348.
22. M. Trhcova, J . Stejskal and J. Prokes, Synth. Met, 101: 1999: 840.
23. K.G. Neoh, M. Y. Pun, E.T. Kang, K.L Tan, Synth. Met., 73: 1995: 209.
24. B.-J. Kim, S.-G. Oh, M.-G. Han, S.-S. Im, Langmuir, 16 : 2000 : 5841.
Received on 09.08.2011 Modified on 17.08.2011
Accepted on 25.08.2011 © AJRC All right reserved